ymt2343esr
Steel Plate
AISI, DIN, JIS, GB
C: 0.35-0.40 Si:0.80-1.10 Mn:0.30-0.50V:0.30-0.50
Forged
Block
Black Primer
High-strength Steel Plate, Wear Resistant Steel, Cold Heading Steel, Mold Steel
Tool Steel Bar
Aluminum, Magnesium, Zine Die Cast, Mold Core
YMT
Container or Metal Framework
Max 500mm thickness
China
7224909090
Product Description



YMT2343R 
is a specialized version of the high-alloy Chromium-Molybdenum-Vanadium Hot 
Work Tool steel.
Engineered for the most demanding high-pressure Light Alloys (Al-Mg) die casting dies, adhering to NADCA #207-2011 PUBLICATION #229 specifications.
Delivered in annealed condition at less than 230HB max. 

Main applications
High pressure Aluminium/Magnesium die casting moulds.
Moulds for low pressure Aluminium die castings.
Moulds for Aluminium gravity die castings.
Plastic injection moulds with optical mirror polishing.

The main features of YMT2343R are:
excellent isotropy
high mechanical properties and strength
high hardenability
high thermal conductivity
high tempering resistance
high thermal stability
high thermal fatigue and hot cracking resistance
excellent fracture toughness in hot and cold conditions
high ductility
high wear and erosion resistance
high oxidation resistance
high ductility

Chemical analysis

AlloyCSiMnCrMo V  
% in wgt0.32-0.40
 
0.80-1.100.30-0.504.80-5.501.20-1.500.30-0.50  

Physical and mechanical properties
Main physical properties
 
 200 °C400°C600°C 
Modulus of elasticity
[MPa]
210183168 
Coefficient of thermal expansion
 [10-6/K]
-11.812.4 
Thermal conductivity
[W/m K]
24.427.128.5 

Main mechanical properties
 
 400°C500°C600°C 
UltimateTensileStrength
 (UTS) [MPa] 
1150950670 
Yield stress (YS) [MPa]900750470 
Soft annealing
 

 
Suggested temperature850°C
HeatingMax 50°C/h
Soaking timeMinimum 120 min from the temperatures settlement
CoolingSlow in the furnace at max 25°C/h to 600°C afterward at room temperature
  
Stress Relieving  
Suggested temperatureFor material in annealed condition: 700-750 °C. For material in H+T condition or after machining: 50°C less than the last tempering
HeatingMax 100 °C/h
Soaking timeMinimum 120 min from the temperature's settlement
CoolingSlow in the furnace at max 25 °C/h to 200°C, afterward at room temperature
  
Hardening 
First pre-heating temperature400 °C
HeatingMax 150 °C/h
Soaking time25 min every 25 mm thickness
Second pre-heating temperature600 °C
HeatingMax 150 °C/h
Soaking time20 min every 25 mm thickness or when (Ts-Tc) < 90 °C
Third pre-heating temperature800 °C
HeatingMax 150 °C/h
Soaking time20 min every 25 mm thickness or when (Ts-Tc) < 90 °C
Austenitizing temperature990-1010°C
Heating> 150°C/h
Soaking timet = ( x + 39 ) / 2 or 30 min
from (Ts-Tc) < 15 °C
CoolingAir, vacuum cooling, salt
bath, polymer in water
First tempering temperature560 - 590 °C
Soaking timet' = 0,8 x + 120
CoolingRoom temperature
Second tempering temperaturehigher than the temperature used for the first temper.
Soaking timet" = 0,8 x + 120
CoolingRoom temperature
Third tempering temperature30-50 °C lower than the max temperature previously used
Soaking timet'" = 0,8 x + 180
CoolingSlow cooling in the furnace up to 250 °C, afterward at room temperature

 